Mga rekomendasyon
NOELSONTMMIOX A-160M/A-320M atbp.
Simulan ang pagbabalangkas
Epoxy modified Alkyd-MIO primer:
| Bahagi A | ||
| Epoxy na binagong alkyd resin | 20 | 50% sa Xylene |
| Micaceous iron oxide gray | 30 | NOELSONTMMIOX A-320M |
| Talc filler | 5 | |
| TIO2 | 3 | Maaari mo ring palitan ng aluminum paste o pangkulay na pigment. |
| Thixatrol ST | 0.5 | |
| Bahagi B | ||
| Epoxy na binagong alkyd resin | 35 | 50% sa Xylene |
| Solvent Oil 100# | 5.5 | |
| Cobalt Dryer, 6% | 0.5 | |
| Anti-balat | 0.5 | |
High solid Epoxy-MIO primer:
| Bahagi A | ||
| Bisphenol A epoxy resins | 14.0 | Epikote 828 (Shell) |
| Urea-formaldehyde resins | 1.5 | Plastopal EBS 400 (BASF) |
| Butyl alcohol | 3.0 | |
| Xylene | 6.0 | |
| Micaceous iron oxide gray | 37 | NOELSONTMMIOX A-320M |
| Zinc phosphate | 15 | NOELSONTMZP 409-3 |
| Talc filler | 5 | |
| TiO2 | 5 | |
| Thixatrol ST | 1 | |
| Butyl alcohol | 2.0 | Idinagdag pagkatapos ng halo |
| Xylene | 10.5 | Idinagdag pagkatapos ng halo |
| Bahagi B | ||
| Epoxy resin hardener | 65 | Cardolite NC 541/90 X |
| Petrolyo dagta | 35 | |
| A/B = 6:1 (ayon sa timbang) | ||